Table 2 Fire properties of developed composites of polyester with BPF and CHAp

From: Cone calorimetric fire properties and thermal analysis of polyester-banana peduncle fibre composite fused with bio-fire retardant additive

Samples

MHRR (KW/m2)

PHRR (KW/m2)

THR (MJ/m2)

MASS loss (g/m2)

TSR (m2/m2)

TSP (m2)

TOC (g)

TTG (s)

ETT (s)

Polyester

223.56

556.54

308.60

14,142.10

9378.20

82.90

206.30

64.00

1445.00

2.5%BPF:2.5%CHAp

223.47

534.19

308.20

13,843.10

8889.20

81.40

203.90

65.00

1540.00

5%BPF:5%CHAp

222.39

516.23

301.20

13,754.50

8579.40

80.60

200.10

75.00

1585.00

7.5%BPF:7.5%CHAp

206.84

501.80

280.90

13,106.00

8161.50

78.90

129.32

80.00

1685.00

10%BPF:10%CHAp

207.57

505.42

207.90

12,580.20

80,582.00

70.90

121.16

82.00

1705.00