From: Green waste recycling of peanuts highly contaminated with aflatoxins in clay brick manufacturing
Run | X1 | X2 | Compressive strength of clay-PA bricks (Model I) | Compressive strength of clay-PB bricks (Model II) |
---|---|---|---|---|
1 | 6.00 | 725.00 | 109.85 | 126.33 |
2 | 35.00 | 725.00 | 5.32 | 6.33 |
3 | 6.00 | 875.00 | 66.27 | 70.09 |
4 | 35.00 | 875.00 | 5.10 | 6.31 |
5 | 0 | 800.00 | 339.30 | 339.30 |
6 | 41.01 | 800.00 | 5.09 | 5.74 |
7 | 20.50 | 693.93 | 13.89 | 14.71 |
8 | 20.50 | 906.07 | 10.35 | 9.00 |
9 | 20.50 | 800.00 | 11.80 | 11.97 |
10 | 20.50 | 800.00 | 12.90 | 11.70 |
11 | 20.50 | 800.00 | 12.00 | 11.50 |
12 | 20.50 | 800.00 | 12.75 | 12.90 |
13 | 20.50 | 800.00 | 12.20 | 12.20 |